Fettling/Deburring/Smoothing Operations
Process | Objective | Finish | Limits to effectiveness | Mode |
Belt Grinding | To remove traces of ingate, parting line, burs, ejector marks and surface defects before bobbing | 60 grit Ra = 1 to 2
400 grit Ra = 0,1 |
Internal areas | Manual
Semi- automatic (carousel) Automatic |
Bobbing | Reduce surface roughness and remove grinding marks | Ra 0,01 to 0,25 | Internal areas | Manual
Semi- automatic (carousel) Automatic |
Vibro Finishing | To reduce roughness and grinding marks. To deburr, radius, polish. |
Ra 0.01 to 0.3 | Internal areas with small dimensions | Semi- automatic
Automatic |
Shot/Grit Blasting | To reduce surface defects. To deburr | Variable | Areas not exposed to the shot direction | Semi- automatic
Automatic |
Where an applied coating is considered necessary the following table gives an indication of the most suitable type of finish for any given application.
Finishing Processes for Zinc Alloy Diecastings
Y= Can achieve desired effect
y= May achieve effect but not usually specified for that reason |
corrosion resistance | aesthetics | colour coding | alter reflectivity | prevent tainting of foodstuff | increase wear resistance | reduce friction | remove sharp edges | increase surface hardness | allow soldering | electrical contact resistance | Improve EMI shielding |
vibratory finishing | Y | Y | Y | |||||||||
shot/grit blasting | y | Y | Y | |||||||||
chemical passivation | Y | y | y | y | Y | |||||||
electrophoretic paint | Y | Y | Y | Y | ||||||||
lacquer (dip/barrel) | Y | Y | Y | |||||||||
zinc plate | Y | Y | ||||||||||
powder coat | Y | Y | Y | y | Y | |||||||
wet paint | Y | Y | Y | y | Y | |||||||
copper plate | y | Y | y | y | Y | y | Y | |||||
brass plating | y | Y | y | y | ||||||||
nickel plate | Y | Y | y | Y | Y | y | y | y | ||||
tin plate | y | y | y | y | y | Y | y | |||||
satin nickel plate | y | Y | Y | y | y | y | ||||||
chromium plate | y | Y | Y | Y | Y | Y | y | |||||
satin chromium plate | y | Y | Y | y | y | y | y | |||||
black chromium plate | y | Y | Y | y | y | y | y | |||||
dry film lubricant | y | y | y | y | Y | Y | ||||||
silver plate | y | Y | Y | y | y | y | y | |||||
gold plate | y | Y | Y | y | y | Y | y | |||||
hard chromium plate | y | y | y | y | Y | Y | Y | |||||
electroless copper | y | y | y | y | Y | y | y | |||||
electroless nickel/phosphorous | y | y | y | Y | Y | Y | y | y | ||||
electroless nickel/ptfe | y | y | y | Y | Y | y |
� � �
Type of Treatment | Maximum class of use advised(See following table) | Properties affected? | Comments | ||
Protec-tion | Decor-ation | Mech | Phys | ||
Chemical Conversion Coatings | |||||
Chromate Passivation | 3-4 | no | no | no | Anticorrosion |
Chemical Black | 1-2 | 1-2 | no | yes | Antireflective |
Phosphate | 1 | no | no | yes | Pretreatment, organic finishes |
Electroless Plating | |||||
Nickel Phosphorous | 4 | no | yes | yes | Hardness, anti-corrosion, friction, electrical contacts |
Nickel PTFE | 4 | no | yes | yes | Friction, wear resistance |
Electroplate | |||||
Silver | 4 | 1 | no | yes | Food contact, anti-corrosion, electrical contacts, RMI, EFI |
Bronze (on Cu+Ni) | 3 | no | no | Appearance, (protect with lacquer from acid attack) | |
White Bronze (on Cu+Ni) | 3 | no | no | Jewellery in contact with the skin | |
Cadmium (on Cu+Ni) | no | yes | yes | Amelioration of corrosion couples | |
Gunmetal (on Cu+Ni) | 3 | no | no | Appearance, (protect with lacquer from acid attack) | |
Chromium (on Cu+Ni) | 4 | 1 to 4 | yes | yes | Appearance, anticorrosion |
Bright | 3 to 4 | 4 | yes | yes | Appearance, anticorrosion |
Satin | 4 | yes | yes | Appearance, anticorrosion | |
Black | 3 | yes | yes | Appearance, anticorrosion | |
Copper | 3 | no | yes | Soldering, food contact | |
Tin Alloys (Sn,Sn-Pb,Sn-Ni) | 4 | no | no | yes | Soldering, wear, friction, food contact |
Brass (on Cu+Ni) | 2 to 3 | no | no | Appearance, (protect with lacquer from acid attack) | |
Nickel (on Cu) | 1 to 4 | 1 to 3 | no | no | Appearance, wear resistance |
Bright, matt, multicoat | 3 | 1 to 4 | no | no | Appearance, wear resistance |
Gold(on Cu+Ni) | 4 | 1 | yes | yes | Appearance, electrical contact |
Palladium (on Cu+Ni) | No | no | yes | Electrical contact | |
Rhodium (on Cu+Ni) | 4 | no | yes | Appearance, stabilisation of brilliance(gold and silver) | |
Zinc+chromate | 4 | no | yes | Appearance, anticorrosion | |
Zinc | 3 | 3 | no | no | Appearance, anticorrosion |
Vacuum Metallizing | |||||
Aluminium | 2 | 1 to 2 | no | yes | Reflectivity, wave guides |
Silver | 2 | 1 to 2 | no | yes | Electrical conductivity |
Gold | 2 | 1 to 2 | no | yes | Infra red reflectivity |
Carbon | 2 | 1 to 2 | yes | yes | Wear, anticorrosion |
Organic Finishes | |||||
Electropaint | 4 | 4 | yes | yes | Anticorrosion |
Wet Paint | |||||
Epoxy | 1 to 2 | 1 to 2 | no | no | Decoration |
Polyurethane | 4 | 4 | yes | no | Decoration, anticorrosion |
Acrylic/Polyurethane | 1 | 1 | no | no | Decoration |
Powder Coating | |||||
Epoxy | 1 to 2 | 1 to 2 | no | no | Decoration |
Epoxy-Polyester | 3 | 3 | yes | no | Decoration, good anticorrosion |
Polyester | 4 | 4 | yes | no | Decoration, good UV resistance, best anticorrosion |
Special Finishes | |||||
Dry Film Lubricants | 4 | no | Low friction, , good dielectric | ||
Plastic Coating | 4 | 4 | Noise and vibration reduction |
�
Exposure Classes
Condition of Use | Class |
Decoration only. Any protection regarded as a bonus | 0 – 1 |
Dry interior: without condensation, interior of dwellings | 0 – 1 |
Damp interior: condensation, kitchens, bathrooms, cellars and workshops, unheated warehouses. | 2 |
Moderate rural outside: Outside in the countryside in moderate climates | 3 |
Moderate outside city: Outside in industrial towns in moderate climates | 3 (4) |
Tropical: Heat and condensation experienced in tropical areas | 4 |
Industrial: Factories and their vicinity. Strong content in the atmosphere of various compounds including SO2 | 4 |
Marine: Coastal atmospheres and on the sea, without being directly in contact with seawater. Corrosion resulting from high relative humidity and salt in the air. | 4 |
Occasional splashing with corrosive materials
Variations in temperature (-40C to +120C): variation in the corrosive conditions Corrosion by various aggressive gases, liquids and solids: |
Tests